[[Image:CoinCellAssembly.png|right|400px]]
[[Image:CoinCellAssembly.png|right|thumb|400px|Figure from Lt. Col. F. John Burpo]] Though some nice micrographs like what you can find on the front page of this module would be great, your TEM results may have revealed nanowires that are not uniform in their appearance or in their gold coating. Fortunately, even ugly-duckling nanowires may serve beautifully when assembled into a battery. The question you'd like to address is if a battery electrode made from gold nanowires (+ some percentage of silver) performs better than a battery made with a solid, gold foil electrode. And having included silver in the templating, how does the % of that metal affect the voltage potential and the charging of the battery? To answer these questions, you will assemble your nanowires into a battery, mixing a known percentage of the active nanowire material, with a small amount of conducting material and a small amount of binding material. The conducting material we'll use is a graphite carbon called “Super P”. The binder is a kind of teflon called polytetrafluoroethylene, or PTFE for short, that will hold the nanowires and carbon conductor together. The nanowires, carbon and teflon will form a flexible film that you'll roll out like cookie dough and that will serve as the electrode (shown in black in this image) for your battery. The electrode will then be moved into a glovebox to be assembled with the lithium and the electrolyte, and pressed into a coin-type casing.


==Protocols==
==Protocols==
All material should be isolated and dried to form a powder. This powder is what will be used to make the battery electrodes.  In all battery electrodes there is a certain percentage of active material, a small amount of conducting material and a small amount of binding material. In these batteries, the conducting material will be a particular type of graphite carbon called “Super P”. The binder is a compound that causes all the powder to stick together and form a flexible film, the binder is teflon (poly(tetrafluoroethylene)—PTFE). These will be mixed at a ratio of 70% active material, 25% Super P, and 5% PTFE.
Some of today's lab protocol will require that we work in small groups in the Belcher lab. We'll be using their balance to measure very small masses of material and their glove box to assemble the batteries. As visitors to their lab, please be respectful of their time, equipment and space.
===Part 1: Examining TEM images===
Images from your TEM grids are [ftp://prism.mit.edu/Burpo/2009-11-25%2020_109%20Lab%20AuNWs/ here]. They are organized with the following numbering scheme:
<center>
{| border="1"
! Lab section
! Team color
! .tif #
|-
|T/R
|Red
|1-4
|-
|
|Green
|5-8
|-
|
|Blue
|9-12
|-
|
|Orange
|13-16
|-
|
|Pink
|17-20
|-
|
|Yellow
|21-24
|-
|
|Purple
|25-28
|-
|W/F
|Pink
|29-32
|-
|
|Purple
|33-36
|-
|
|Green
|37-40
|-
|
|Red
|41-44
|-
|
|Blue
|45-48
|}
</center>
When you are not busy measuring the materials to assemble in your batteries, please examine these images and prepare one as if it were to be a figure in a research article (see the FNT assignment, below). Also please post a summary comment about the images to [http://openwetware.org/index.php?title=Talk:20.109%28F09%29:_Mod_3_Day_4_Battery_assembly&action=edit the talk page] of today's wiki.


#Measure the mass of powder and add to a clean agate mortar, determine the mass of Super P and PTFE to add based on this mass.
===Part 2: Electrode Composition===
You'll need to make some careful mass measurements and then mix the nanowires: carbon (= Super P): teflon (PTFE) at the correct ratio of 70% nanowires:25% Super P:5% PTFE. All material should be isolated and ground to form a powder. This powder is what will be used to make the battery electrodes. 
#In small groups, visit the Belcher lab (2nd floor of building 16). The mortar with your nanowires will be there drying in their vacuum oven. Bring your notebooks, a calculator, and carry (don't wear) some latex gloves.
#Use the Belcher lab's [http://www.dartmouth.edu/~chemlab/techniques/a_balance.html analytical balance] to measure the mass of nanowire powder. Add this mass to a clean mortar.
#Grind the nanowires for 5 minutes. You and your lab partner(s) can take turns grinding. While you're not grinding determine the mass of Super P and PTFE to be add based on the mass of the nanowires.
#Measure out Super P and add to mortar. Do not add PTFE yet!
#Measure out Super P and add to mortar. Do not add PTFE yet!
#Grind thoroughly with mortar and pestle for about 15 minutes.   
#Grind thoroughly with mortar and pestle for about 20 minutes.   
#Add PTFE and mix together, use the pestle to press the mixture into a flat sheet that is all one piece.
#Add PTFE and mix together, use the pestle to press the mixture into a flat sheet that is all one piece.
#Transfer to a stainless steel plate and roll out the electrode to form a uniform electrode.
#Transfer to a stainless steel plate and roll out the electrode to form a uniform electrode.
#Once rolled, transfer to the stainless steel cutting plate and use a circle cutter to make an electrode.   
#Once rolled, transfer to the stainless steel cutting plate and use a circle cutter to make an electrode.   
#Measure mass of electrode and determine the theoretical capacity of the electrode. Co3O4 has a theoretical capacity of ~890mAh/g, FePO4•H2O has a capacity of 143 mAh/g (milli Amp hours per gram).
#Measure mass of the electrode (you'll need this to calculate your battery's capacity).  
#The electrodes have to dry before they can be assembled into a battery so before the next lab, this will be done for you in the glove box in the Belcher lab. Today you will have an opportunity to see a demonstration of the assembly with materials that have been prepared in advance.


==For Next Time==
==For Next Time==
==Reagents==
#Prepare a figure of your nanowires from one of the TEM images that has been posted. The figure should be "publication ready," i.e. with all the traditional elements found for figures in a research article. If you'd like to examine other figures from TEM studies, consider some of the Belcher lab's publications, e.g. Nano Lett., 2005, 5 (7), pp 1429–1434 [[DOI: 10.1021/nl050795d]]
#Read the introductory material for [http://openwetware.org/wiki/20.109%28F09%29:_Mod_3_Day_5_Battery_testing the battery testing lab,] and then, based on the mass of the active electrode material you've made, determine the number of mA to apply in order to fully discharge the battery in 10 hours. Use the loading factor of 51 mA/g, a value that is in accordance with previously tested gold nanowire electrodes.
#You should be well on your way to your final presentations of a research idea. Review the required elements for your presentation that are noted [http://openwetware.org/wiki/20.109%28F09%29:_Mod_3_Day_6_Oral_presentations here.]

Latest revision as of 09:59, 7 December 2009


20.109(F09): Laboratory Fundamentals of Biological Engineering

Home        People        Schedule Fall 2009        Assignments        Lab Basics        OWW Basics       
DNA Engineering        System Engineering        Biomaterials Engineering              

Battery Assembly

Introduction

Figure from Lt. Col. F. John Burpo
Though some nice micrographs like what you can find on the front page of this module would be great, your TEM results may have revealed nanowires that are not uniform in their appearance or in their gold coating. Fortunately, even ugly-duckling nanowires may serve beautifully when assembled into a battery. The question you'd like to address is if a battery electrode made from gold nanowires (+ some percentage of silver) performs better than a battery made with a solid, gold foil electrode. And having included silver in the templating, how does the % of that metal affect the voltage potential and the charging of the battery? To answer these questions, you will assemble your nanowires into a battery, mixing a known percentage of the active nanowire material, with a small amount of conducting material and a small amount of binding material. The conducting material we'll use is a graphite carbon called “Super P”. The binder is a kind of teflon called polytetrafluoroethylene, or PTFE for short, that will hold the nanowires and carbon conductor together. The nanowires, carbon and teflon will form a flexible film that you'll roll out like cookie dough and that will serve as the electrode (shown in black in this image) for your battery. The electrode will then be moved into a glovebox to be assembled with the lithium and the electrolyte, and pressed into a coin-type casing.

Protocols

Some of today's lab protocol will require that we work in small groups in the Belcher lab. We'll be using their balance to measure very small masses of material and their glove box to assemble the batteries. As visitors to their lab, please be respectful of their time, equipment and space.

Part 1: Examining TEM images

Images from your TEM grids are here. They are organized with the following numbering scheme:

Lab section Team color .tif #
T/R Red 1-4
Green 5-8
Blue 9-12
Orange 13-16
Pink 17-20
Yellow 21-24
Purple 25-28
W/F Pink 29-32
Purple 33-36
Green 37-40
Red 41-44
Blue 45-48

When you are not busy measuring the materials to assemble in your batteries, please examine these images and prepare one as if it were to be a figure in a research article (see the FNT assignment, below). Also please post a summary comment about the images to the talk page of today's wiki.

Part 2: Electrode Composition

You'll need to make some careful mass measurements and then mix the nanowires: carbon (= Super P): teflon (PTFE) at the correct ratio of 70% nanowires:25% Super P:5% PTFE. All material should be isolated and ground to form a powder. This powder is what will be used to make the battery electrodes.

  1. In small groups, visit the Belcher lab (2nd floor of building 16). The mortar with your nanowires will be there drying in their vacuum oven. Bring your notebooks, a calculator, and carry (don't wear) some latex gloves.
  2. Use the Belcher lab's analytical balance to measure the mass of nanowire powder. Add this mass to a clean mortar.
  3. Grind the nanowires for 5 minutes. You and your lab partner(s) can take turns grinding. While you're not grinding determine the mass of Super P and PTFE to be add based on the mass of the nanowires.
  4. Measure out Super P and add to mortar. Do not add PTFE yet!
  5. Grind thoroughly with mortar and pestle for about 20 minutes.
  6. Add PTFE and mix together, use the pestle to press the mixture into a flat sheet that is all one piece.
  7. Transfer to a stainless steel plate and roll out the electrode to form a uniform electrode.
  8. Once rolled, transfer to the stainless steel cutting plate and use a circle cutter to make an electrode.
  9. Measure mass of the electrode (you'll need this to calculate your battery's capacity).
  10. The electrodes have to dry before they can be assembled into a battery so before the next lab, this will be done for you in the glove box in the Belcher lab. Today you will have an opportunity to see a demonstration of the assembly with materials that have been prepared in advance.

For Next Time

  1. Prepare a figure of your nanowires from one of the TEM images that has been posted. The figure should be "publication ready," i.e. with all the traditional elements found for figures in a research article. If you'd like to examine other figures from TEM studies, consider some of the Belcher lab's publications, e.g. Nano Lett., 2005, 5 (7), pp 1429–1434 DOI: 10.1021/nl050795d
  2. Read the introductory material for the battery testing lab, and then, based on the mass of the active electrode material you've made, determine the number of mA to apply in order to fully discharge the battery in 10 hours. Use the loading factor of 51 mA/g, a value that is in accordance with previously tested gold nanowire electrodes.
  3. You should be well on your way to your final presentations of a research idea. Review the required elements for your presentation that are noted here.