=How to Create a PDMS-Stamp from Silicone/Araldite Mold=


==Preparation of PDMS mixture==
* with pipette boy and 5ml stripette pour ~4g of elastomer into a cup
* with micropipette (1000µl) add one tenth of elastomer mass (~0.4g) of linker fluid to the cup
* mix well with stripette
* degass for 30min-60min
==Preparation of PDMS membrane==
* pour degassed mixture onto wafer placed in petri dish with aluminium foil
* pour just enough to cover the waver
* use [[Christian Niederauer/Notebook/RacingBacteria/Stock/Leveling_Petri_Dish | Leveling Petri Dish]] to ensure constant thickness
* araldite wafer: cure it for 3-4 hours in oven at 60°C
* silicon wafer: cure it for 2 hours in oven at 80°C for
* peel off membrane from wafer surface with forceps
* cut out the pattern but '''leave enough space around it'''
==Final Processing==
* punch holes with 2mm coring tool at the desired connection points under dissection microscope (tip: target the hole with coring tool under microscope, then put the stamp onto one finger with alufoil between stamp and finger and push/turn until you feel the coring tool on your skin)
* [[Christian Niederauer/Notebook/RacingBacteria/Protocols/Plasma_Cleaning | plasma clean]] the treated face of the stamp and a coverslip and press them together with alufoil in order to prevent contamination
===If the stamp is too thin===
'''BEFORE PUNCHING HOLES'''
* take a slice of PDMS with bigger or same area than the stamp
* [[Christian Niederauer/Notebook/RacingBacteria/Protocols/Plasma_Cleaning | plasma clean]] unshaped face of stamp and extra slice and stick them together
* now punch desired holes with 2mm coring tool