User:Alicia Rasines Mazo/Notebook/CHEM-582 Experimental Chemistry II/2015/04/15: Difference between revisions

From OpenWetWare
Jump to navigationJump to search
No edit summary
(fix raw html notebook nav)
 
Line 2: Line 2:
|-
|-
|style="background-color: #EEE"|[[Image:owwnotebook_icon.png|128px]]<span style="font-size:22px;"> Project name</span>
|style="background-color: #EEE"|[[Image:owwnotebook_icon.png|128px]]<span style="font-size:22px;"> Project name</span>
|style="background-color: #F2F2F2" align="center"|<html><img src="/images/9/94/Report.png" border="0" /></html> [[{{#sub:{{FULLPAGENAME}}|0|-11}}|Main project page]]<br />{{#if:{{#lnpreventry:{{FULLPAGENAME}}}}|<html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>[[{{#lnpreventry:{{FULLPAGENAME}}}}{{!}}Previous entry]]<html>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;</html>}}{{#if:{{#lnnextentry:{{FULLPAGENAME}}}}|[[{{#lnnextentry:{{FULLPAGENAME}}}}{{!}}Next entry]]<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html>}}
|style="background-color: #F2F2F2" align="center"|[[File:Report.png|frameless|link={{#sub:{{FULLPAGENAME}}|0|-11}}]][[{{#sub:{{FULLPAGENAME}}|0|-11}}|Main project page]]<br />{{#if:{{#lnpreventry:{{FULLPAGENAME}}}}|[[File:Resultset_previous.png|frameless|link={{#lnpreventry:{{FULLPAGENAME}}}}]][[{{#lnpreventry:{{FULLPAGENAME}}}}{{!}}Previous entry]]&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;}}{{#if:{{#lnnextentry:{{FULLPAGENAME}}}}|[[{{#lnnextentry:{{FULLPAGENAME}}}}{{!}}Next entry]][[File:Resultset_next.png|frameless|link={{#lnnextentry:{{FULLPAGENAME}}}}]]}}
|-
|-
| colspan="2"|
| colspan="2"|

Latest revision as of 00:54, 27 September 2017

Project name Main project page
Previous entry      

Tasks for April 15

  • To run DSC on epoxy/amine (JA-230 and 400) and epoxy/mine/tiO2 cured films
  • To coat copper electrodes with epoxy/TiO2 (JA-400) and carry out corrosion testing
  • To work on final presentation

Preparation of epoxy/TiO2 coatings for corrosion test

  • 1.6260 g of JA-400 amine
  • 0.50119 g of TiO2
  • 3.48357 g of epoxy

Vortexed and gently stirred at 65°C before applying onto copper electrodes and curing for 4 h.