<u>Procedure:</u>


==Data==
A PVOH (MW=22000, 0.5g, 5ml) film was synthesized using the procedure from 8/29/2012. Before allowing the film to dry, 0.25mL of glutaraldehyde was added with stirring for ~5 minutes. This solution was then left to dry.
* Add data and results here...


==Notes==
The clay was exchanged with surfactant in 100 and 50 percents. To create the 100% exchange solution: 2.00 g of clay and 0.7390g of HdMe<sub>2</sub>Im<sup>+</sup> (surfactant) were dissolved in a 50/50 mixture of H<sub>2</sub>O/ethanol (25mL each) and left to stir for one week. The 50% exchange solution was created with the same parameters except using half the amount of HdMe<sub>2</sub>Im<sup>+</sup> (0.3690g).
This area is for any observations or conclusions that you would like to note.


A solution of 1.04g iron(II) chloride, 0.5g iron sulfate, 2g of clay, and 40mL of H<sub>2</sub>O was prepared. To precipitate iron oxide out of the solution, sodium hydroxide (2.67g in 10mL H<sub>2</sub>O) was added dropwise with stirring. The solution was then filtered using vacuum filtration and left to dry.


Use categories like tags. Change the "Course" category to the one corresponding to your course. The "Miscellaneous" tag can be used for particular experiments, as instructed by your professor. Please be sure to change or delete this tag as required so that the categories remain well organized.
==Data==
 
mass of filter paper: 0.33684 g
[[Category:Course]]
[[Category:Miscellaneous]]


==Notes==
N/A





Revision as of 12:40, 5 October 2012

Experimental Chemistry <html><img src="/images/9/94/Report.png" border="0" /></html> Main project page
<html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>Previous entry<html>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;</html>Next entry<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html>


Objective

Synthesize polymer film with the addition of gluteraldehyde, exchange clay in solution with a surfactant, synthesize iron oxide

Description

Procedure:

A PVOH (MW=22000, 0.5g, 5ml) film was synthesized using the procedure from 8/29/2012. Before allowing the film to dry, 0.25mL of glutaraldehyde was added with stirring for ~5 minutes. This solution was then left to dry.

The clay was exchanged with surfactant in 100 and 50 percents. To create the 100% exchange solution: 2.00 g of clay and 0.7390g of HdMe2Im+ (surfactant) were dissolved in a 50/50 mixture of H2O/ethanol (25mL each) and left to stir for one week. The 50% exchange solution was created with the same parameters except using half the amount of HdMe2Im+ (0.3690g).

A solution of 1.04g iron(II) chloride, 0.5g iron sulfate, 2g of clay, and 40mL of H2O was prepared. To precipitate iron oxide out of the solution, sodium hydroxide (2.67g in 10mL H2O) was added dropwise with stirring. The solution was then filtered using vacuum filtration and left to dry.

Data

mass of filter paper: 0.33684 g