Part 1: Preparing solutions for coating AuNP with Silica
1) dissolve 0.716g PVP (10kg/mol) in 10mL water (0.00716M)
2) Dissolve 0.42mL NH<sub>4</sub>OH (29.3wt% NH<sub>3</sub> in H<sub>2</sub>O) in 9.58mL Ethanol (200 proof) (4.2vol%)
NOTE: TES solution will be prepared immediately prior to use to minimize exposure
Part 2: Preparing ZnPPIX solutions





Revision as of 07:40, 5 June 2013

Project name <html><img src="/images/9/94/Report.png" border="0" /></html> Main project page
<html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>Previous entry<html>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;</html>Next entry<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html>

Objectives

Procedures

Part 1: Preparing solutions for coating AuNP with Silica

1) dissolve 0.716g PVP (10kg/mol) in 10mL water (0.00716M) 2) Dissolve 0.42mL NH4OH (29.3wt% NH3 in H2O) in 9.58mL Ethanol (200 proof) (4.2vol%)

NOTE: TES solution will be prepared immediately prior to use to minimize exposure

Part 2: Preparing ZnPPIX solutions