User:Allison K. Alix/Notebook/Thesis Research/2013/08/13

From OpenWetWare
Jump to navigationJump to search
The printable version is no longer supported and may have rendering errors. Please update your browser bookmarks and please use the default browser print function instead.
Project name <html><img src="/images/9/94/Report.png" border="0" /></html> Main project page
<html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>Previous entry<html>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;</html>Next entry<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html>

Scaled up Silica-Coating Procedure

Original: 1mL AuNP & MHA solution/2μL TES/0.125mL NH4OH/5mL 2-propanol

1) Re-scale to use 9mL AuNP/MHA solution

New: 9mL AuNP&MHA solution/18uL TES/1.125mL NH4OH/45mL 2-propanol

2) Stir solutions for one hour to allow reaction to proceed

3) Centrifuge solutions at 4000 rpm for one hour

4) Re-suspend particles in water

Calculations

Original concentration of AuNP/MHA solution is 4.7nM

4.7nM(9mL)=55.143mL(x)

x= 0.767nM

0.767x10^-9moles/L x 1L/1000mL x 36mL = 2.7612 x 10^-11 moles AuNP total

2.7612 x 10^-11 moles AuNP x 6.02 x 10^23 particles/mole = 1.66 x 10^13 total Au nanoparticles

  • We want a 5nM solution

5x10^-9 moles/L x 1L/1000mL x 6.02x10^23 particles/mole = 3.01 x 10^12 particles/mL

1.66 x 10^13 particles / x = 3.01 x10^12 particles/1 mL

x = 5.52mL

Dilute AuNP in 5.52mL water after removing supernantant

5.52mL/24 vials = 230uL per vial.

DNA Attachment Procedure 1

Adapted from Silica Coated, Au/Ag Striped Nanowires for Bioanalysis

1) Mix 300uL AuNP@SiO2, 30uL APS, 470uL ethanol. Stir for 30 minutes.

2) Centrifuge solution at 9100rpm for 30 second intervals. Rinse 3 times with ethanol and twice with sodium phosphate buffer (SPB), pH=9. Redisperse in 800uL SPB.

3) In a seperate solution, mix 2mg Sulfo-SMCC with 800uL SPB. Vortex to dissolve.

4) Add 800uL Sulfo-SMCC with 800uL Au@SiO2-NH2. Stir for one hour.

5) Centrifuge at 9100rpm, twice with SPB and twice with potassium phosphate buffer (KPB), pH=7.4. Redisperse in 400uL KPB

6) Add 50uL 5uM DNA to 400uL Sulfo-SMCC activated Au@SiO2 solution. Stire for 1 hour

7) Rinse three times with KPB, Redisperse in 150uL KPB.

DNA Attachment Procedure 2

Adapted from Gold and Silica-Coated Gold Nanoparticles as Thermographic Labels for DNA Detection

1) Mix 1mL 5nM AuNP@SiO2 with 5uL 1mM APS. Stir for 1hr.

2) Reduce thiol DNA to HS-DNA using DTT. Dissolve 2mg Sulfo-SMCC in 2mL 0.05M KPB. Mix 250uL solution with 250uL 3uM DNA. Mix for 1 hour

3) Centrifuge DNA/Sulfo-SMCC solution for 20 minutes at 13,200rpm. Remove excess Sulfo-SMCC and redisperse DNA in 250uL PBS.

4) Mix 250uL Sulfo-SMCC activated DNA with AuNP@SiO2-NH2 solution. Stir for 2 hours. Centrifuge for 1 hour @ 4000rpm.

5) Resuspend in water (250uL?, 500uL)

Data

Above are spectra showing pure AuNP (23.5nM), AuNP coated in silica (5nM) and NH2 functionalized Au@SiO2 (5nM). We will assume an even silica coating due to the observed 11nm peak shift of the Au@Si02 which is characteristic of silica coated particles.