==Procedure==
==Procedure==
'''Creating the Gold Stock Solution'''
'''Creating the Gold Stock Solution'''
#  
# Add 0.0506 g of HAuCl<sub>4</sub>·3H<sub>2</sub>O were added to a 50 mL volumetric flask and filled with distilled water.
# The final concentration of gold stock was 2.57 mM.


'''Creating the Lysozyme Solution'''
'''Creating the Lysozyme Solution'''
#
# Add


'''Creating the Myoglobin Solution'''
'''Creating the Myoglobin Solution'''
#
# Add


'''Synthesizing Lysozyme AuNP and Myoglobin AuNP'''
'''Synthesizing Lysozyme AuNP and Myoglobin AuNP'''

Revision as of 10:00, 29 October 2013

Project name <html><img src="/images/9/94/Report.png" border="0" /></html> Main project page
<html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>Previous entry<html>&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;</html>Next entry<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html>

Objective

Analysis and synthesis of more protein-AuNP materials. Each group will have a different task. One (set) of groups will be doing AA on their samples from last weed (HRP-AuNPs and pepsin-AuNPs) and this week (Myoglobin-AuNPs and HRP-AuNPs). Another (set) will take UV-Vis absorbance of their samples (this week and last week). The final (set) will synthesize new protein-AuNPs.

Procedure

Creating the Gold Stock Solution

  1. Add 0.0506 g of HAuCl4·3H2O were added to a 50 mL volumetric flask and filled with distilled water.
  2. The final concentration of gold stock was 2.57 mM.

Creating the Lysozyme Solution

  1. Add

Creating the Myoglobin Solution

  1. Add

Synthesizing Lysozyme AuNP and Myoglobin AuNP Solutions with the following Au:protein ratio were synthesized:

Gold to Lysozyme Ratio

  • 30
  • 50
  • 70
  • 90
  • 110
  • 130
  • 150
  • 170
  • 190
  • 210

Gold to Myoglobin Ratio

  • 10
  • 15
  • 25
  • 30
  • 35
  • 40
  • 45
  • 50
  1. As seen in Figure 1, the corresponding amount of protein was added to a 50 mL volumetric flask and filled with distilled water. The samples were made in small test tubes and capped with aluminum foil.
  2. The samples were heated at 80°C for 4 hours.

Notes

  • The final gold concentration in the solutions was 0.25 mM.