<u>Making films with PDMS and glutaraldehyde</u> | |||
Film 1 | |||
# 0.5 g of PVOH was dissolved in 5 mL of water and was placed on a hotplate | |||
# 1 mL of glutaraldehyde was added to the solution under the hood. | |||
# The mixture was allowed to stir for about 3 minutes. | |||
# The film was poured into a dish and was left under the hood over the weekend | |||
Film 2 | |||
# 0.4 g PVOH and 0.1262 g PDMS were dissolved in 5 mL of water on a hot plate. | |||
# Once dissolved, 1 mL of glutaraldehyde was added to the PVOH/PDMS | |||
# The mixture was allowed to stir without heat for 3 minutes | |||
# The film was poured into a dish and was left under the hood over the weekend | |||
<u>Making clay films</u> | |||
# | |||
==Data== | ==Data== |
Revision as of 07:08, 3 October 2012
Experimental Chemistry | <html><img src="/images/9/94/Report.png" border="0" /></html> Main project page <html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>Previous entry<html> </html>Next entry<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html> |
ObjectiveTo conduct clay-CuSO4 exchange, remake films with PDMS and glutaraldehyde, and prepare films containing clay (Na-MT and 100% CEC) DescriptionMaking films with PDMS and glutaraldehyde Film 1
Data
Notes
|