| + | The three PVOH/glutaraldehyde films prepared last class were crosslinked | ||
==Description== | ==Description== | ||
| - | + | <u>Crosslinking Glutaraldehyde Films</u> | |
| - | + | ||
| - | + | # Allow the PVOH film containing glutaraldehyde to dry completely. | |
| - | + | # Prepare a solution of 100 mL H<sub>2</sub>O, 2 mL concentrated H<sub>2</sub>SO<sub>4</sub>, and 20 g Na<sub>2</sub>SO<sub>4</sub> in a 150 mL beaker. (solution is referred to as glutaraldehyde fixant) | |
| + | # Place stir bar in beaker and a Buchner funnel top (cap) over the stir bar | ||
| + | # Heat solution to 70°C (temperature on hotplate should be about 160) | ||
| + | # Place film in solution for one hour. | ||
| + | # Prepare 100 mL of a 1% HCl solution in a 150 mL beaker. Place a stir bar and an inverted buchner funnel into beaker. | ||
| + | # Heat HCl solution to 70°C | ||
| + | # Remove film from glutaraldehyde fixant and rinse with distilled water. | ||
| + | # Place film into HCl solution for 30 minutes. | ||
| + | # Prepare 0.2 M sodium bicarbonate solution. (1.68 g in 100 mL) | ||
| + | # After 30 minutes, remove the film from the HCl solution and place into the sodium bicarbonate solution (at room temperature) for about 15 minutes. | ||
| + | # Use tweezers to remove the film from the sodium bicarbonate solution. | ||
| + | # Rinse film with deionized water and dry film on paper towel. | ||
| - | |||
| - | + | ==Data== | |
| - | + | ||
| + | * No data was collected today | ||
| + | |||
| + | ==Notes== | ||
| + | |||
| + | * The dye film made last class has a medium yellow color | ||
| + | * The Na-MT film still looks like it formed with one side thicker than the other side (was not uniform). | ||
| + | * On Monday, need to prepare a porphyrin-HCl film with NaCl for crosslinking. | ||