User:Madeleine Y. Bee/Notebook/CHEM-581 Experimental Chemistry/2014/09/26: Difference between revisions
From OpenWetWare
No edit summary |
No edit summary |
||
Line 16: | Line 16: | ||
====Start New Film Synthesis==== | ====Start New Film Synthesis==== | ||
*PVA Exchanged-Clay Film | *AMT's PVA Exchanged-Clay Film | ||
*#Add 7mL of water to | *#Add 7mL of water to 1.0114 g of 22,000MW polyvinyl alcohol and 1.0290 g of exchanged NaMT in a glass vial | ||
*#Stir the solution with constant heating at 75C until the polymer is dissolved and the clay is dispersed (~15 minutes) | *#Stir the solution with constant heating at 75C until the polymer is dissolved and the clay is dispersed (~15 minutes) | ||
*#Cool the solution to room temperature | *#Cool the solution to room temperature | ||
Line 24: | Line 24: | ||
*#Pour solution into a teflon dish to dry until the next class | *#Pour solution into a teflon dish to dry until the next class | ||
*PVA Exchanged-Clay Film | *BEM's PVA Exchanged-Clay Film | ||
*#Add 7mL of water to | *#Add 7mL of water to 1.0290 g of 22,000MW polyvinyl alcohol and 0.1105 g of exchanged NaMT in a glass vial | ||
*#Stir the solution with constant heating at 75C until the polymer is dissolved and the clay is dispersed (~15 minutes) | *#Stir the solution with constant heating at 75C until the polymer is dissolved and the clay is dispersed (~15 minutes) | ||
*#Cool the solution to room temperature | *#Cool the solution to room temperature |
Revision as of 09:51, 26 September 2014
CHEM 581: Experimental Chemistry | <html><img src="/images/9/94/Report.png" border="0" /></html> Main project page <html><img src="/images/c/c3/Resultset_previous.png" border="0" /></html>Previous entry<html> </html>Next entry<html><img src="/images/5/5c/Resultset_next.png" border="0" /></html> |
September 26, 2014ProceduresFinishing Cation-Exchanged Clay Films
Start New Film Synthesis
|