Objectives
- Crosslink PVOH films.
- Make more PVOH (MW 130000) films with strong acid and maleic or succinic acid.
- Run solubility tests on crosslinked and uncrosslinked PVOH films.
- Run FTIR and DSC on PVOH films.
PVOH (MW 22,000) Films
| '
| No acid
| HCl
| H3PO4
|
| No acid | 1.0115 | 0.5181 | 1.0054
|
| 10 wt% maleic acid | | 0.5181 |
|
| 15 wt% maleic acid | | | 1.0054
|
| 10 wt% succinic acid | | 0.5163 |
|
| 15 wt% succinic acid | | | 1.0125
|
PVOH (MW 130,000 Films
| '
| No acid
| HCl
| H3PO4
|
| No acid | | 0.9964 | 1.0855
|
| 10 wt% maleic acid | | 1.0106 (mass of maleic acid: 0.1071) |
|
| 15 wt% maleic acid | | | 1.0373 (mass of maleic acid: 0.1556)
|
| 10 wt% succinic acid | | 1.0215 (mass of succinic acid: 0.1021) |
|
| 15 wt% succinic acid | | | 1.0178 (mass of succinic acid: 0.1528)
|
Solubility of PVOH Films
- 0.1023 g of uncrosslinked PVOH (MW 22000), 15 wt% maleic acid, H3PO4 was dissolved in 75 mL H2O.
- The viscosity of the solution was tested:
| Trial
| Time [s]
|
| 1 | 246.67
|
| 2 | 253.48
|
| 3 | 250.68
|
DSC on PVOH Films
- About 3 mg ± 20% PVOH film was placed in a DSC pan.
- Uncrosslinked PVOH (MW 22000) + 15% maleic acid + H3PO4
- Pan mass: 49.42 mg
- Sample mass: 3.13 mg
- Uncrosslinked PVOH (MW 22000) + 15% succinic acid + H3PO4
- Pan mass: 51.02 g
- Sample mass: 3.15 g
- Procedure:
- Equilibrate at 20.00°C.
- Ramp 20.00°C/min to 240.00°C.
- Ramp 20.00°C/min to 20.00°C.
- Repeat steps 2 and 3 one time.
Notes
- Films were crosslinked in the oven at 120°C for 90 minutes.
- Crosslinked PVOH films became more rigid and changed color from transparent to faintly yellow-brown.
- The viscometer used for previous tests was discovered to be cracked. A new viscometer was subsequently used.
|