Objective
- Perform gold nanoparticle(AuNP) synthesis to obtain purple homogeneous solution using 15.5 μM Bovine Serum Albumin (BSA), 2.9 mM Chloroauric Acid (HAuCl4), H2O, and Tris.
Description
Tube 1: 0.1 mL BSA, 0.1 mL HAuCl4, 0.8 mL H2O.
Tube 2: 0.1 mL BSA, 0.1 mL HAuCl4, 0.8 mL Tris Buffer (pH 9.36).
Tube 3: 0.1 mL BSA, 0.05 mL HAuCl4, 0.85 mL H2O.
Tube 4: 0.1 mL BSA, 0.05 mL HAuCl4, 0.85 mL Tris Buffer (pH 9.36).
- Tubes placed in heat block set at 80 degrees celsius, for 2 hours.
- Heat block was turned off after 2 hours to facilitate gradual decrease in temperature.
Data
- Tube 1: Purple protein fiber aggregation, Molar ratio of Au/BSA = 187
- Tube 2: Clear solution, Molar ratio of Au/BSA = 187
- Tube 3: Purple solution (similar to experiment performed on 9/28), Molar ratio of Au/BSA = 98.4
- Tube 4: Clear solution, Molar ratio of Au/BSA = 98.4
Notes
|